Common Quality Problems And Solutions Of SMC Composite Molded Products
Oct 15, 2024
Leave a message
The SMC composite molding process is one of the most efficient FRP/composite molding processes. There are many advantages of SMC composite molding process, such as: accurate product size, smooth surface, good repeatability of product appearance and size, complex structure can also be molded at one time, and secondary processing does not need to damage the product.
Molding equipment: hydraulic press, should have
(1) Adequate countertops
(2) Sufficient stroke
(3) Sufficient pressure
(4) Reasonable speed
(5) Reasonable structural form
Common quality problems and how to solve them
Although the SMC composite molding process is one of the most efficient in the FRP/composite molding process. The SMC composite molding process also has many advantages, such as: accurate product size, smooth surface, good repeatability of product appearance and size, complex structure can also be molded at one time, and secondary processing does not need to damage the product. However, there will also be defects in the molding production process of SMC composites, which are mainly manifested in the following aspects:
1) Lack of materials
Lack of material refers to the fact that the SMC composite compression molded parts are not completely filled, and the production parts are mostly concentrated at the edges of SMC products, especially the roots and tops of the corners.
Mechanism and countermeasures:
(1) After the SMC material is thermoplasticized, the melt viscosity is large, and there is not enough time, pressure and volume to fill the mold cavity before the cross-linking curing reaction is completed.
(2) The storage time of SMC composite molded material is too long, and the styrene volatilization is excessive, resulting in a significant decrease in the fluidity of SMC composite molded material.
(3) The resin paste is not soaked with fibers. During molding, the resin paste cannot drive the fiber to flow, resulting in a shortage of material. The most direct solution to the shortage of materials caused by the above reasons is to remove these molded materials when cutting materials.
(4) Insufficient feeding amount causes material shortage. The solution is to increase the amount of material appropriately.
(5) The molded material is wrapped with too much air and a large amount of volatiles. The solution is to increase the number of exhausts appropriately; Appropriately increase the feeding area and clean the mold at a certain time; Increase the molding pressure appropriately.
(6) The pressurization is too late, and the molded material has been cross-linked and cured before filling the mold cavity.
(7) If the mold temperature is too high, the cross-linking curing reaction is advanced, and the temperature should be appropriately cooled.
Common quality problems and solutions of SMC composite molded products [Chengdu Zhengxi hydraulic press] sharing
2) Stomata
There are regular or irregular small holes on the surface of the product, which are mostly generated at the top and middle thin walls of the product. Mechanism and countermeasures:
(1) The SMC composite molding material is wrapped in a large amount of air and the volatile content is large, and the exhaust is not smooth; The thickening effect of SMC material is not good, and the gas cannot be effectively driven out. The above causes can be effectively controlled by increasing the number of exhaust times and cleaning the mold.
(2) If the feeding area is too large, it can be controlled by appropriately reducing the feeding area. In practice, human factors may also cause trachoma. For example, if the pressure is too early, it may make the gas wrapped in the molded material difficult to discharge, resulting in surface defects of porosity on the surface of the product.
3) Warping deformation
The main causes are uneven curing of the molded material and shrinkage of the product after demoulding. Mechanism and countermeasures:
During the resin curing reaction, the chemical structure changes, causing volume shrinkage, and the uneven curing causes the product to warp towards the first cured side. Secondly, the thermal expansion coefficient of the product is larger than that of the steel mold. When the product is cooled, its unidirectional shrinkage is greater than that of the mold. To this end, the following methods are used to solve the problem:
(1) Reduce the temperature difference between the upper and lower molds, so that the temperature distribution is as uniform as possible;
(2) Use cooling fixtures to limit deformation;
(3) Appropriately increase the molding pressure, increase the structural compactness of the product, and reduce the shrinkage rate of the product;
(4) Appropriately extend the holding time and eliminate internal stress.
(5) Adjust the curing shrinkage of SMC material.
4) Blistering
A semicircular bulge on the surface of the cured product. Mechanism and countermeasures:
It may be that the curing of the material is incomplete, the local temperature is too high or the volatile content in the material is large, and the semicircle on the surface of the product bulges due to the air collection between the sheets.
(1) Appropriately increase the molding pressure
(2) Extend the holding time
(3) Reduce the mold temperature
(4) Reduce the discharging area
5) The surface color of the product is uneven
Mechanism and countermeasures:
(1) The mold temperature is uneven and the local temperature is too high, so the mold temperature should be properly controlled;
(2) The fluidity of the molded material is poor, resulting in uneven fiber distribution, which can generally increase the molding pressure and increase the fluidity of the melt;
(3) In the process of color paste blending, the pigment and resin cannot be well miscited.
In fact, molding a good product is mainly determined by four elements: press, material, mold and operator. Therefore, a good press can mold a good product, although it is not the only condition, it must be a prerequisite.